PP Orient Energy T30H Resin
PP Orient Energy T30H Resin
Material Introduction: PP Orient Energy T30H is high‑flow homopolymer polypropylene, specially designed for high‑speed injection‑molding thin‑wall food containers and daily‑use articles. It meets food‑contact compliance such as GB 4806.6 with good cost‑performance, while its low‑temperature toughness is relatively weak.
Main Applications
Extruded flat yarn: woven bags, packing straps, ropes, carpet base fabrics.
Injection‑molding: household goods, toys and general daily‑use products.
Performance Parameters
| Performance Category | Test Item | Test Condition | Reference Value | Unit | Reference Standard | Remarks & Interpretation |
|---|---|---|---|---|---|---|
| Basic Properties | Melt Flow Rate(MFR) | 230℃/2.16 kg | 2.5‑3.5 | g/10 min | ASTM D1238 | Homopolymer PP grade. |
| Density | ‑ | 0.90‑0.91 | g/cm³ | ASTM D1505 | ‑ | |
| Mechanical Properties | Tensile Yield Strength | ‑ | ≥30‑32 | MPa | ASTM D638 | ‑ |
| Flexural Modulus | ‑ | ≥1100‑1200 | MPa | ASTM D790 | ‑ | |
| Izod Impact Strength | 23℃ | ≥32‑39 | J/m | ASTM D256 | Room‑temperature impact. | |
| Thermal Properties | Heat‑Distortion Temperature(HDT) | 0.45 MPa / 0.46 MPa, non‑annealed | To be confirmed | ℃ | ASTM D648 | Data pending confirmation. |
| Other Properties | Rockwell Hardness | R‑scale | ≥80‑90 | ‑ | ASTM D785 | Surface hardness. |
Injection‑Molding Process Parameters
| Process Item | Suggested Range / Description | Remarks |
|---|---|---|
| Drying treatment | Generally unnecessary; dry at 80℃ for about 1 h under poor storage condition | PP low‑moisture‑absorption feature. |
| Barrel rear zone(feed section) | 160‑200℃ | Prevent thermal degradation. |
| Barrel middle zone(compression section) | 180‑220℃ | ‑ |
| Barrel front zone(metering section) | 200‑240℃ | ‑ |
| Nozzle temperature | 200‑240℃ | ‑ |
| Melt temperature | ‑ | 220‑280℃ |
| Mold temperature | 20‑70℃,recommended 40‑60℃ | Crystallization mainly determined by mold temperature. Low temperature: poor surface, weld‑line and flow‑mark risks; high temperature will cause warpage. |
| Injection pressure | 80‑140 MPa(800‑1400 bar); higher pressure for thin‑wall & complex parts, up to 180 MPa(1800 bar) except partial thin‑wall packaging containers. | ‑ |
| Holding pressure | 30%‑60% of injection pressure | Prevent sink mark and excessive shrinkage; holding time accounts for approx. 30% of cycle time. |
| Back pressure | 5‑20 MPa(50‑200 bar) | ‑ |
| Injection speed | Medium injection speed; high‑speed injection required for thin‑wall packaging containers. | ‑ |
| Screw speed | High screw speed(linear velocity 1.3 m/s) is permitted | Complete plasticization before cooling phase finishes. |
| Runner & Gate | Pin‑point gate or multi‑point gate; heated hot‑runner, insulated hot‑runner. Gate shall be set at thick‑wall position of product, otherwise severe shrinkage defect easily occurs. | Mold‑design suggestion. |