GPPS BASF‑Yangzi 158K

GPPS BASF‑Yangzi 158K

GPPS BASF‑Yangzi 158K is a general‑purpose polystyrene with balanced properties. It is widely applied for its high transparency, high strength, good heat resistance, excellent rigidity and easy‑processing characteristics.

Main Applications

Medical laboratory ware, cosmetic packaging, food containers (e.g. cake trays), CD/DVD cases, transparent injection‑molded parts, extruded sheets, etc.

Property Data

表格

Property Category Test Item Test Standard Unit Typical Value / Range
Physical Properties Density ISO 1183 g/cm³ 1.05
  Melt Flow Rate (MFR) ISO 1133 (200 °C / 5 kg) cm³/10min or g/10min 3
  Water Absorption ISO 61 % <0.1
Mechanical Properties Tensile Yield Stress ISO 527 MPa 55
  Elongation at Break ISO 527 % 3
  Tensile Modulus ISO 527 MPa 3300
  Flexural Strength ISO 178 MPa 103
  Charpy Un‑notched Impact Strength (23 °C) ISO 179/1eU kJ/m² 17
  Charpy Notched Impact Strength (23 °C) ISO 179/1eA kJ/m² 3
  Rockwell Hardness (Scale L) ASTM D785 100
Thermal Properties Vicat Softening Temperature (B/50) ISO 306 (50 N, 50 °C/h) °C 101
  Heat Deflection Temperature (HDT, 0.45 MPa) ISO 75 °C 98
Optical Properties Appearance Highly transparent
Electrical Properties Volume Resistivity IEC 6093 Ω·cm >10¹⁴
Flammability UL 94 Rating UL 94 HB
Others Molding Shrinkage % 0.3‑0.6

Injection Molding Parameters

表格

Process Parameter Reference Range / Recommendation Remarks
Drying 60‑80 °C, 2‑3 hours (subject to storage conditions) PS has low moisture absorption. Drying is recommended if recycled content is present, ambient humidity is high or storage is abnormal.
Barrel Temperature 180‑260 °C Adjust within range according to part geometry.
Mold Temperature 10‑60 °C Higher mold temperature improves surface gloss and reduces internal stress.
Melt Temperature Polystyrene features a broad melting‑processing window.
Injection Pressure Depends on part shape and wall thickness; adjust according to practical conditions.

Extrusion Process

表格

Process Parameter Reference Range / Recommendation Remarks
Drying Pre‑drying or vented vacuum screw is recommended Even minor moisture may cause defects during extrusion.
Processing Temperature 200‑240 °C  

Note: All data above is for reference only

!