POM Asahi Kasei TENAC‑C Z3510
POM Asahi Kasei TENAC‑C® Z3510
POM 日本旭化成 Z3510,高粘度共聚 POM‑C,高分子量,高强度、高刚性,韧性优于普通通用 POM,尺寸稳定性、耐磨、抗蠕变、耐疲劳表现突出。
Main Applications
Automotive: fuel‑pump assemblies, fuel‑caps, seat‑belt components and other interior functional parts requiring high rigidity & dimensional‑stability. Electrical & electronic: gears, bearings and structural parts for washing‑machines, refrigerators, shavers and other household appliances. Precision machinery: high‑precision gears, bearings, cams, screws demanding high‑wear‑resistance and low‑friction. Consumer & industrial goods: window‑frame / shutter parts, toys, game‑console components and industrial fittings with high rigidity & dimensional‑stability requirements。
Physical‑Mechanical‑Thermal‑Electrical Properties
表格
| Property Category | Item | Test Standard | Value | Unit |
|---|---|---|---|---|
| Physical Properties | Density | ISO 1183 / ASTM D‑792 | 1.41 | g/cm³ |
| Water absorption(24 h) | ASTM D‑570 | 0.20 | % | |
| MFR (190 ℃ / 2.16 kg) | ISO 1133 | 2.8 | g/10 min | |
| Molding shrinkage (flow) | ISO 294‑4 / ASTM D‑955 | 1.6‑2.0 | % | |
| Molding shrinkage (cross‑flow) | ISO 294‑4 | 1.6‑2.0 | % | |
| Mechanical Properties | Tensile modulus | ISO 527‑2 | 2650 | MPa |
| Tensile yield stress | ISO 527‑2 | 63.0 | MPa | |
| Tensile strength (break) | ASTM D‑638 | 61 | MPa | |
| Elongation at break | ISO 527‑2 / ASTM D‑638 | 60 / 75 | % | |
| Flexural modulus | ASTM D‑790 | 2600 | MPa | |
| Flexural strength | ASTM D‑790 | 88 | MPa | |
| Charpy notched impact 23 ℃ | ISO 179/1eA | 9.0 | kJ/m² | |
| Izod notched impact 23 ℃ | ASTM D‑256 | 78 | J/m | |
| Rockwell hardness M‑scale | ASTM D‑785 | 78 | — | |
| Taber abrasion (1000 cycles) | ASTM D‑1044 | 14 | mg | |
| Thermal Properties | HDT (1.8 MPa, unannealed) | ISO 75‑2/A | 95.0 | ℃ |
| HDT (1.8 MPa, unannealed) | ASTM D‑648 | 110 | ℃ | |
| HDT (0.45 MPa, unannealed) | ISO 75‑2/B | 156 | ℃ | |
| HDT (0.45 MPa, unannealed) | ASTM D‑648 | 158 | ℃ | |
| CLTE (flow) | ASTM E‑831 | 1.0×10⁻⁴ | cm/cm/℃ | |
| Melting point(DSC) | DSC | 165 | ℃ | |
| Flammability | UL94(0.81 mm / 1.50 mm) | UL 94 | HB | — |
Injection‑Molding Parameters
表格
| Process Stage | Parameter | Recommended Range | Unit | Remarks |
|---|---|---|---|---|
| Pre‑drying | Drying temperature | 80‑90 | ℃ | Must dry sufficiently; desiccant dryer recommended, avoid silver‑streaks & bubbles旭化成。 |
| Drying time | 2‑4 | h | ||
| Target residual moisture | <0.15 | % | ||
| Barrel temperature | Rear zone | 180‑200 | ℃ | Narrow processing window, strictly<220 ℃, overheating releases formaldehyde gas。 |
| Middle zone | 190‑210 | ℃ | ||
| Front zone | 195‑215 | ℃ | ||
| Nozzle temperature | 190‑210 | ℃ | Slightly lower or close to front‑zone, prevent drooling。 | |
| Melt temperature | 195‑215 | ℃ | ||
| Mold temperature | 80‑100 | ℃ | Higher mold‑temp improves crystallization, gloss and reduces sink‑marks。 | |
| Injection parameters | Injection pressure | 80‑130 | MPa | Adjust by part geometry & wall‑thickness。 |
| Hold‑up pressure | 40‑80 | MPa | Sufficient hold‑pressure to compensate shrinkage。 | |
| Back pressure | 0.5‑2.0 | MPa | Keep low; excessive back‑pressure causes shear‑overheat degradation。 | |
| Injection speed | Medium | — | Avoid excessive shear heat from too‑fast filling or short‑shot from too‑slow filling。 | |
| Screw speed | 50‑100 | rpm | Do not over‑spin screw to limit shear heat。 | |
| Post‑treatment | Annealing | Optional | — | Normally unnecessary; anneal high‑precision parts to release internal‑stress。 |
| Barrel residence time | <20 | min | Avoid long‑term high‑temperature retention。 | |
| Shutdown procedure | Short‑term stop | Cool barrel below 150 | ℃ | Long‑term shutdown purge barrel with PE / PP。 |
Note: All data for reference only, subject to official TDS and COA。