POM Mitsubishi Iupital F20‑03
POM Mitsubishi Iupital® F20‑03(Thailand)
POM Mitsubishi F20‑03 is medium‑viscosity general‑purpose copolymer‑acetal(POM‑C) injection grade. Balanced mechanical performance, good dimensional‑stability, wide service‑temperature range, excellent wear‑resistance and chemical‑resistance, widely‑used universal grade for precision mechanical components。
Main Applications
Automotive: gears, bearings, transmission parts, fuel‑system components, seat‑belt parts, inner‑door handles, window‑regulator mechanisms. Electrical & electronic: electrical components, connectors, switch parts, structural & transmission parts for printer / copier OA‑equipment. Precision machinery & industrial components: high‑precision gears, bearings, cams, screws, levers, pulleys, sprockets, pipe‑valve parts with low‑friction & wear‑resistance requirement. Consumer goods: toys, sports‑equipment (ski‑board, sailing‑hardware), zippers, fasteners, lighters, thermostat‑timer components。
Physical‑Mechanical‑Thermal‑Electrical Properties
| Property Category | Item | Test Standard | Value | Unit |
|---|---|---|---|---|
| Physical Properties | Density | ISO 1183 / ASTM D‑792 | 1.41 | g/cm³ |
| Equilibrium water absorption(23 ℃, 50 %RH) | ISO 62 / ASTM D‑570 | 0.22 | % | |
| MFR (190 ℃ / 2.16 kg) | ISO 1133 / ASTM D‑1238 | 9.0 | g/10 min | |
| Molding shrinkage(flow,3 mm) | ASTM D‑955 / Internal | 2.0 | % | |
| Mechanical Properties | Tensile yield strength | ISO 527‑2 / ASTM D‑638 | 61.0‑64.0 | MPa |
| Elongation at break | ISO 527‑2 / ASTM D‑638 | 30‑35 | % | |
| Tensile modulus | ISO 527‑2 | 2900 | MPa | |
| Flexural strength | ISO 178 / ASTM D‑790 | 87.0‑90.0 | MPa | |
| Flexural modulus | ISO 178 / ASTM D‑790 | 2550‑2600 | MPa | |
| Charpy notched impact 23 ℃ | ISO 179/1eA | 6.5‑7.0 | kJ/m² | |
| Izod notched impact 23 ℃ | ASTM D‑256 | 64 | J/m | |
| Rockwell hardness M‑scale | ASTM D‑785 | 80 | — | |
| Thermal Properties | HDT (1.8 MPa) | ISO 75‑2/A / ASTM D‑648 | 100‑110 | ℃ |
| HDT (0.45 MPa) | ISO 75‑2/B / ASTM D‑648 | 156‑158 | ℃ | |
| Melting temperature | ISO 11357‑3 | 165‑166 | ℃ | |
| CLTE (flow direction) | ISO 11359‑2 / ASTM D‑696 | 1.1×10⁻⁴ | cm/cm/℃ | |
| Electrical Properties | Volume resistivity | IEC 60093 / ASTM D‑257 | 1×10¹⁴ | Ω·cm |
| Surface resistivity | IEC 60093 / ASTM D‑257 | 1×10¹⁶ | Ω | |
| Dielectric strength (3 mm) | IEC 60243‑1 / ASTM D‑149 | 19 | kV/mm | |
| Dielectric constant (1 MHz) | ASTM D‑150 / IEC 60250 | 3.70‑3.90 | — | |
| Dissipation factor (1 MHz) | ASTM D‑150 / IEC 60250 | 0.0070 | — | |
| Flammability | UL94 (0.8 mm) | UL 94 | HB | — |
Injection‑Molding Parameters
| Process Stage | Parameter | Recommended Range | Unit | Remarks |
|---|---|---|---|---|
| Pre‑drying | Drying temperature | 80‑100 | ℃ | Drying recommended; avoid bubbles & silver‑streaks, improve dimension & surface quality。 |
| Drying time | 3‑4 | h | ||
| Target moisture content | <0.1‑0.2 | % | ||
| Barrel temperature | Rear zone | 170‑180 | ℃ | Narrow thermal processing window. Melt temperature ≤220 ℃, overheat causes formaldehyde decomposition。 |
| Middle zone | 180‑190 | ℃ | ||
| Front zone | 190‑200 | ℃ | ||
| Nozzle temperature | 180‑210 | ℃ | Close to / slightly lower than front‑zone temperature to prevent drooling。 | |
| Melt temperature | 190‑210 | ℃ | ||
| Mold temperature | 60‑80 | ℃ | Higher mold‑temperature improves crystallization, gloss and reduces sink‑marks。 | |
| Injection parameters | Injection pressure | 50‑100 | MPa | Adjust by part geometry & wall‑thickness。 |
| Hold‑up pressure | — | MPa | Adequate hold‑pressure required to compensate shrinkage。 | |
| Back pressure | Low value | MPa | High back‑pressure induces shear‑overheat degradation。 | |
| Injection speed | Medium, multi‑stage | — | Too‑slow: flow marks; too‑fast: jetting & shear heat。 | |
| Screw speed | 80‑120 | rpm | Avoid excessive rotational speed to reduce shear heat。 | |
| Barrel residence time | <20‑30 | min | Keep residence time short to prevent thermal degradation。 | |
| Shutdown procedure | Short‑term stop | Cool barrel below 150 | ℃ | Long‑term shutdown: fully purge barrel with PE / PP。 |
| Purge note | PE / PP | — | Must purge halogen‑containing polymers before POM processing to prevent violent chemical reaction。 | |
| Post‑treatment | Annealing (optional) | — | — | Relieve residual stress for high‑precision parts working under non‑ambient service condition。 |
Note: All data for reference only, subject to official TDS and COA。