POM Zhonghao K90 is medium‑viscosity copolymer‑acetal(POM‑C) injection grade. Balanced mechanical property, standard flowability, good dimensional‑stability, broad service‑temperature window, good chemical‑resistance, excellent wear‑resistance & self‑lubrication, widely used for general‑purpose mechanical components。
Note: K90 is base grade;K90‑A is enhanced thermal‑stabilized version, adding high‑efficiency thermal stabilizer, less formaldehyde precipitation & mold deposit during long‑time production;mechanical parameters are basically consistent, K90‑A is more suitable for continuous mass production。
Main Applications
Automotive: gears, bearings, fuel‑system components, seat‑belt parts. Electrical & electronic: electrical components, connectors, structural & transmission parts for printer / copier OA‑equipment. Precision machinery & industrial parts: high‑precision gears, bearings, cams, screws, levers, pulleys with low‑friction & wear‑resistance requirement. Consumer goods: toys, sports‑equipment, zippers, fasteners, lighters; pipe fittings, conveyor accessories, water‑boiler parts, pump housing, strainers, faucet components。
Physical‑Mechanical‑Thermal Properties
| Property Category | Item | Test Standard | Value | Unit |
|---|---|---|---|---|
| Physical Properties | Density | ASTM D‑792 | 1.41 | g/cm³ |
| Water absorption (23 ℃,24 h) | ASTM D‑570 | 0.22 | % | |
| MFR (190 ℃ / 2.16 kg) | ASTM D‑1238 | 9.0 | g/10 min | |
| Molding shrinkage | — | 2.0 | % | |
| Mechanical Properties | Tensile strength (yield) | ASTM D‑638 | 62 | MPa |
| Elongation at break | ASTM D‑638 | 60 | % | |
| Flexural strength | ASTM D‑790 | 91.5 | MPa | |
| Flexural modulus | ASTM D‑790 | 2650 | MPa | |
| Izod notched impact (23 ℃) | ASTM D‑256 | 6.5 | kJ/m² | |
| Tensile impact strength | ASTM D‑1822 | 110 | ft·lb/in² | |
| Rockwell hardness M‑scale | ASTM D‑785 | M80 | — | |
| Thermal Properties | HDT (1.8 MPa) | ASTM D‑648 | 110 | ℃ |
| HDT (0.45 MPa) | ASTM D‑648 | 158 | ℃ | |
| Melting temperature | DSC | 165 | ℃ | |
| CLTE (20‑80 ℃) | ASTM E‑831 | 13×10⁻⁵ | cm/cm/℃ | |
| Flammability | UL94 (0.8 mm) | UL 94 | HB | — |
Injection‑Molding Parameters
| Process Stage | Parameter | Recommended Range | Unit | Remarks |
|---|---|---|---|---|
| Pre‑drying | Drying temperature | 80‑90 | ℃ | Drying recommended, avoid bubble & silver‑streak, improve dimension & surface quality。 |
| Drying time | 2‑4 | h | ||
| Barrel temperature | Rear zone | 150‑180 | ℃ | Narrow thermal window. Melt temperature ≤220 ℃, overheat causes formaldehyde decomposition。 |
| Middle zone | 170‑190 | ℃ | ||
| Front zone | 180‑200 | ℃ | ||
| Nozzle temperature | 170‑190 | ℃ | Slightly lower than front‑zone temperature to prevent drooling。 | |
| Melt temperature(POM‑C) | 190‑210 | ℃ | Typical working range for copolymer POM。 | |
| Mold temperature | 80‑100 | ℃ | Higher mold‑temperature improves crystallization, gloss and reduces sink‑marks。 | |
| Injection parameters | Injection pressure | 40‑130 | MPa | Higher for thin‑wall parts。 |
| Hold‑up pressure | Close to injection pressure | MPa | Sufficient hold‑pressure compensates shrinkage。 | |
| Back pressure | 0.5‑2.0(minimum preferred) | MPa | High back‑pressure brings shear‑overheat degradation。 | |
| Injection speed | Medium‑fast | — | Too‑slow: flow marks; too‑fast: jetting & shear heat。 | |
| Screw speed | 100‑150 | rpm | Avoid excessive screw‑speed; keep small cushion。 | |
| Barrel residence time | <20 | min | Only 7 min maximum retention under 240 ℃。 | |
| Shutdown procedure | Short‑term stop | Cool barrel below 150 | ℃ | Long‑term shutdown: fully purge with PE / PP。 |
| Purge note | PE / PP | — | Must purge halogen‑containing polymers before POM processing to prevent violent reaction。 | |
| Post‑treatment | Annealing(optional) | — | — | Relieve residual stress for high‑precision non‑ambient‑service parts。 |