POM DuPont Delrin 500P

POM DuPont Delrin® 500P

POM DuPont Delrin® 500P is medium‑viscosity homopolymer‑acetal(POM‑H) injection grade. It provides high rigidity, high strength and excellent wear‑resistance, good dimensional‑stability, fair chemical‑resistance, self‑lubricity and broad service‑temperature range, widely‑used general‑purpose base grade for Delrin series。

Main Applications

Automotive: fuel‑pump assemblies, fuel‑cap, seat‑belt components, handle‑parts, power‑window parts, pipe fittings, sliders. Electrical & electronic: gears, bearings and structural parts for home‑appliance timers, keyboard, audio‑video devices. Precision‑machinery & industrial components: gears, bearings, cams, screws, levers, pulleys, sprockets, valve‑pipe parts, fasteners and engineering fittings. Consumer goods: zippers, toys, sports‑equipment, lighters; extruded sheets, strips and tubes。

Physical‑Mechanical‑Thermal‑Electrical Properties

Property Category Item Test Standard ASTM ISO Unit
Physical Properties Density ASTM D‑792 / ISO 1183 1.42 1.42 g/cm³
  Water absorption (24 h immersion) ASTM D‑570 / ISO 62 0.25 1.4(2 mm) %
  Water absorption (50 %RH equilibrium) ASTM D‑570 / ISO 62 0.22 0.30 %
  MFR (190 ℃ / 2.16 kg) ASTM D‑1238 / ISO 1133 9.0 15.0 g/10 min
  Molding shrinkage (flow) — / ISO 294‑4 2.2‑2.4 2.0 %
  Molding shrinkage (transverse) — / ISO 294‑4 1.9 %
Mechanical Properties Tensile yield strength 23℃ ASTM D‑638 / ISO 527‑2 69 71.0 MPa
  Elongation at break ASTM D‑638 / ISO 527‑2 35 30 %
  Tensile modulus ASTM D‑638 / ISO 527‑2 3360 3100 MPa
  Flexural strength ASTM D‑790 / ISO 178 97 80.0(3.5%strain) MPa
  Flexural modulus ASTM D‑790 / ISO 178 3090 2950 MPa
  Izod notched impact 23℃ ASTM D‑256 / ISO 180/1A 81 9.0 J/m;kJ/m²
  Compressive strength(10 %strain) ASTM D‑695 123 MPa
  Rockwell hardness M‑scale ASTM D‑785 / ISO 2039‑2 94 92
Thermal Properties HDT (1.8 MPa) ASTM D‑648 / ISO 75‑2/A 136 95.0
  HDT (0.45 MPa) ASTM D‑648 / ISO 75‑2/B 172 160
  Melting point ASTM D‑2133 / ISO 11357‑3 175 178
  CLTE (flow direction) ASTM D‑696 / ISO 11359‑2 10.4‑14.9×10⁻⁵ 1.1E‑4 cm/cm/℃
Electrical Properties Volume resistivity ASTM D‑257 / IEC 60093 1×10¹⁵ 2.0×10¹⁴ Ω·cm
  Dielectric strength(2.3 mm) ASTM D‑149 / IEC 60243‑1 19.7 44 kV/mm
  Dielectric constant(1 MHz) ASTM D‑150 / IEC 60250 3.7 3.80
Flammability UL94 UL 94 HB HB

Injection‑Molding Parameters

Process Stage Parameter Recommended Range Unit Remarks
Pre‑drying Pre‑treatment Optional, pre‑heat recommended No mandatory drying; 80 ℃ pre‑heat improves dimensional‑stability.
Barrel temperature Rear zone 150‑180 Narrow processing window. Melt shall never exceed 220 ℃, otherwise formaldehyde decomposition occurs.
  Middle zone 170‑190  
  Front zone 180‑200  
  Nozzle temperature 170‑190 Slightly lower than front‑zone temperature to prevent drooling.
  Melt temperature 190‑210  
  Mold temperature 80‑100 Higher mold‑temperature improves crystallization, gloss and reduces sink‑marks.
Injection parameters Injection pressure 40‑130 MPa Adjust by wall‑thickness.
  Hold‑up pressure Close to injection pressure MPa Adequate hold‑pressure compensates shrinkage and sink‑marks.
  Back pressure 0.5‑2.0(minimum preferred) MPa High back‑pressure causes shear‑overheat degradation.
  Injection speed Medium Process strategy: medium pressure, medium speed, low melt temperature, high mold‑temperature.
  Screw speed 100‑150 rpm Avoid excessive screw‑speed; keep small cushion to reduce shear heat.
  Barrel residence time <20 min Short residence time required.
Shutdown procedure Short‑term stop Cool barrel below 150 Long‑term shutdown: fully purge barrel with PE / PP.
Post‑treatment Annealing(optional) For high‑precision parts working under non‑ambient condition, relieve residual stress.

Note: All data for reference only, subject to official TDS and COA。