POM DuPont Delrin 588P
POM DuPont Delrin® 588P
POM DuPont Delrin® 588P is a well‑balanced homopolymer‑acetal grade. It is famous for good stiffness and wear‑resistance, combined with outstanding impact‑resistance, favorable dimensional stability and chemical‑resistance。
Main Applications
Office‑automation equipment: mainly for OA‑device gears. Automotive industry: automotive components. Electrical & electronic: timer assemblies for washing‑machines and juicers. Consumer & others: toys, sports‑equipment, power‑tool accessories。
Physical‑Mechanical‑Thermal‑Electrical Properties
| Property Category | Item | Test Standard | Typical Data | Unit |
|---|---|---|---|---|
| Physical Properties | Density | ASTM D‑792 | 1.42 | g/cm³ |
| Water absorption | ASTM D‑570 | 0.36 | % | |
| Molding shrinkage (flow direction) | ASTM D‑570 | 1.8‑2.1 | % | |
| Mechanical Properties | Tensile yield stress @23 ℃ | ASTM D‑638 | 71 | MPa |
| Tensile yield stress @‑55 ℃ | ASTM D‑638 | 109 | MPa | |
| Tensile yield stress @70 ℃ | ASTM D‑638 | 45 | MPa | |
| Tensile yield stress @100 ℃ | ASTM D‑638 | 28 | MPa | |
| Tensile yield stress @122 ℃ | ASTM D‑638 | 21 | MPa | |
| Tensile breaking strain @23 ℃ | ASTM D‑638 | 56 | % | |
| Tensile breaking strain @‑55 ℃ | ASTM D‑638 | 29 | % | |
| Tensile breaking strain @70/100/122 ℃ | ASTM D‑638 | >60 | % | |
| Flexural strength @23 ℃ | ASTM D‑790 | 105 | MPa | |
| Flexural strength @‑55 ℃ | ASTM D‑790 | 177 | MPa | |
| Flexural strength @70 ℃ | ASTM D‑790 | 54 | MPa | |
| Flexural strength @100 ℃ | ASTM D‑790 | 35 | MPa | |
| Flexural strength @122 ℃ | ASTM D‑790 | 25 | MPa | |
| Flexural modulus @23 ℃ | ASTM D‑790 | 3270 | MPa | |
| Flexural modulus @‑55 ℃ | ASTM D‑790 | 4330 | MPa | |
| Flexural modulus @70 ℃ | ASTM D‑790 | 1480 | MPa | |
| Flexural modulus @100 ℃ | ASTM D‑790 | 900 | MPa | |
| Flexural modulus @122 ℃ | ASTM D‑790 | 630 | MPa | |
| Izod notched impact @23 ℃ | ASTM D‑256 | 68‑75 | J/m | |
| Izod un‑notched impact @23 ℃ | ASTM D‑256 | >1500 | J/m | |
| Compressive stress (1 % strain) @23 ℃ | ASTM D‑695 | 28 | MPa | |
| Compressive stress (10 % strain) @23 ℃ | ASTM D‑695 | 105 | MPa | |
| Shear strength @23 ℃ | ASTM D‑732 | 64 | MPa | |
| Rockwell hardness R‑Scale | ASTM D‑785 | 121 | — | |
| Rockwell hardness M‑Scale | ASTM D‑785 | 87 | — | |
| Thermal Properties | HDT (0.46 MPa) | ASTM D‑648 | 168 | ℃ |
| HDT (1.82 MPa) | ASTM D‑648 | 125 | ℃ | |
| Melting point | ASTM D‑2133 | 175 | ℃ | |
| CLTE ‑40~29 ℃ | ASTM D‑696 | 10.1 | 10⁻⁵ m/m·℃ | |
| CLTE 29~60 ℃ | ASTM D‑696 | 12.3 | 10⁻⁵ m/m·℃ | |
| CLTE 60~104 ℃ | ASTM D‑696 | 14.1 | 10⁻⁵ m/m·℃ | |
| CLTE 104~150 ℃ | ASTM D‑696 | 15.5 | 10⁻⁵ m/m·℃ | |
| Electrical Properties | Volume resistivity @23 ℃ | ASTM D‑257 | 10¹⁵ | Ω·m |
Injection Molding Parameters
| Process Stage | Parameter | Recommended Range | Unit | Remarks |
|---|---|---|---|---|
| Pre‑drying | Drying temperature | >80 | ℃ | Low moisture absorption (0.2‑0.5 %). Drying is recommended for wet raw material to stabilize production and surface quality. |
| Drying time | >2 | h | ||
| Barrel temperature | Rear zone | 150‑180 | ℃ | Homopolymer‑POM has very narrow processing window (~10 ℃). Do NOT exceed 250 ℃, otherwise irritant formaldehyde gas will be generated by decomposition. |
| Middle zone | 170‑190 | ℃ | ||
| Front zone | 180‑200 | ℃ | ||
| Nozzle temperature | Slightly lower than front‑zone temperature | ℃ | Prevent drooling. | |
| Melt temperature(POM‑H) | 190‑230 | ℃ | Typical range for homopolymer‑POM. | |
| Mold temperature | 80‑105 | ℃ | Higher mold temperature improves crystallization, dimensional stability, surface gloss and reduces sink marks. | |
| Injection parameters | Injection pressure | 700‑1200 | bar | Adjust according to part geometry and wall‑thickness. |
| Hold‑up pressure | — | — | Proper hold‑pressure is required to compensate high volumetric shrinkage (~17 %) and avoid sink marks. | |
| Injection speed | Medium‑to‑high | — | ||
| Back pressure | As low as possible (max 200 bar) | bar | High back‑pressure causes thermal‑shear degradation. | |
| Runner & gate | Gate type | Any type | — | For submarine gate: adopt short‑type. Hot‑tip runner is preferred for homopolymer POM. |
| Screw | Screw type | Mutant‑type screw | — | Mutant‑type screw is recommended. |
| Nozzle | Nozzle type | Straight‑through nozzle | — | Straight‑through nozzle preferred. |
| Barrel residence time | As short as possible | min | Long residence inside barrel leads to degradation. | |
| Shutdown procedure | Short‑term shutdown | Drop barrel temperature to 150 | ℃ | Thoroughly purge barrel for long‑term shutdown. |
| Barrel purging material | PE / PP | — | Turn off heating, move screw forward. Keep barrel & screw clean. After halogen‑containing / acidic polymers, purge fully with PE before POM processing to avoid violent chemical reaction. | |
| Post‑treatment | Annealing (if required) | — | — | Thermal stress‑relief annealing is needed for high‑quality parts working under non‑ambient conditions. |
Note: All data above is for reference only!