POM YUNTIANHUA GF‑25

POM YUNTIANHUA GF‑25

POM YUNTIANHUA GF‑25 is 25 % glass‑fiber‑reinforced copolymer acetal. It delivers high stiffness, elevated heat‑deflection temperature, excellent dimensional stability and low molding shrinkage.

Main Applications

Automotive: engineering & industrial fittings, automotive components (under‑hood parts, valve parts, accelerator pedal etc.). Precision mechanical & industrial parts: high‑stiffness gears, bearings, cams, conveyor components requiring high‑precision, wear‑resistance and low‑friction. Consumer & others: furniture structural parts.

Physical Properties

Property Category Item Test Standard Typical Data Unit
Physical Properties Density ISO 1183 1.60 g/cm³
  Water absorption (23℃,24h) ISO 62 0.60 %
  MFR (190℃/2.16kg) ISO 1133 6.0 g/10min
Mechanical Properties Tensile yield strength (23℃) ISO 527‑2 130 MPa
  Elongation at break (23℃) ISO 527‑2 2.5 %
  Tensile modulus (23℃) ISO 527‑2 8000 MPa
  Flexural strength (23℃) ISO 178 180 MPa
  Flexural modulus (23℃) ISO 178 7500 MPa
  Charpy notched impact (23℃) ISO 179/1eA 7.0 kJ/m²
Thermal Properties HDT (1.8 MPa) ISO 75‑2/A 160
Others UL94 rating UL94 HB

Injection Molding Parameters

Process Stage Parameter Recommended Range Unit Remarks
Pre‑treatment Drying temperature 100‑120 Drying recommended for better dimension & appearance, avoid bubbles/silver streaks
  Drying time 2‑4 h  
Injection Rear zone 160‑180 Narrow processing window; strictly avoid>230℃, formaldehyde gas will be generated by decomposition
  Middle zone 170‑200  
  Front zone 180‑210  
  Nozzle temperature 180‑210 Slightly lower or close to front zone to prevent drooling
  Melt temperature 190‑210  
  Mold temperature 60‑90 Higher mold temp improves crystallization, dimensional stability, gloss & reduces sink marks
  Injection pressure Adjust by part geometry & wall thickness  
  Hold‑up pressure Proper hold‑pressure to reduce sink marks  
  Back pressure Keep low Excessive back‑pressure causes shear‑heating degradation
  Injection speed Optimize according to product Slow speed causes ripple; excessive speed brings jet mark & shear degradation
  Screw speed Keep moderate rpm Avoid excessive shear heat leading to material decomposition
  Barrel residence time <20‑30 min Short residence required to prevent decomposition
  Short‑term shutdown Drop barrel temp to 150 Purge barrel thoroughly for long‑term shutdown
  Barrel purging material PE / PP Must purge with PE/PP after halogen‑containing polymers to prevent violent reaction
Post‑treatment Annealing (optional) For high‑quality non‑ambient‑use parts To release internal stress

Note: All information above is for reference only!

  • toolbar
  • toolbar
  • toolbar
  • toolbar