POM YUNTIANHUA M90

POM YUNTIANHUA M90

POM YUNTIANHUA M90 is medium‑viscosity, standard‑flow copolymer acetal with well‑balanced overall performance. It delivers good dimensional stability, excellent comprehensive mechanical properties, wide service temperature range, outstanding chemical resistance and wear resistance, suitable for a wide range of general‑purpose mechanical parts.

Main Applications

Automotive: hood components, wheel parts, valves, exterior parts, automotive electronics. Electrical & electronic: gears, bearings and structural components for home appliances such as washing‑machine & juicer parts, timer assemblies, keyboard & switch components. Precision mechanical & industrial parts: gears, bearings, cams, screws, levers, pulleys, sprockets, pipe valves and other high‑precision, wear‑resistant, low‑friction structural components. Consumer & others: toys, sports goods and thin‑wall articles.

Physical Properties

Property Category Item Test Standard Typical Data Unit
Physical Properties Density ISO 1183 1.41 g/cm³
  Water absorption (23℃,24h) ISO 62 0.60‑0.70 %
  MFR (190℃/2.16kg) ISO 1133 9.0 g/10min
Mechanical Properties Tensile yield strength (23℃) ISO 527‑2 62 MPa
  Elongation at break (23℃) ISO 527‑2 30‑50 %
  Tensile modulus (23℃) ISO 527‑2 2700 MPa
  Flexural strength (23℃) ISO 178 61 MPa
  Flexural modulus (23℃) ISO 178 2400‑2600 MPa
  Charpy notched impact (23℃) ISO 179/1eA 6.0‑7.0 kJ/m²
  Izod notched impact (23℃) ISO 180/1A 7.5 kJ/m²
  Rockwell Hardness (M‑scale) ISO 2039‑2 M82(R114)
Thermal Properties HDT (1.8 MPa) ISO 75‑2/A 115
  Vicat A50 (10 N) ISO 306 A50 163
  Vicat B50 (50 N) ISO 306 B50 150
  Melting point ISO 3146 172
  Linear thermal expansion coefficient ASTM D‑696 11×10⁻⁵ K⁻¹
  Max continuous service temperature 100
Electrical Properties Volume resistivity IEC 60093 10¹⁵ Ω·cm
  Surface resistivity IEC 60093 10¹⁵ Ω
  Dielectric strength (20℃) IEC 60243 25 kV/mm
  Dielectric constant (20℃,1kHz) IEC 60250 3.9
  Dissipation factor (20℃,1MHz) IEC 60250 85×10⁻⁴
Others UL94 rating(0.75 mm) UL94 HB
  Molding shrinkage‑flow (24h,4mm) 2.8‑2.9 %
  Molding shrinkage‑cross (24h,4mm) 2.1‑2.4 %

Injection Molding Parameters

Process Stage Parameter Recommended Range Unit Remarks
Pre‑treatment Drying temperature 80‑90 Low‑hygroscopic; drying recommended for better dimension & appearance, avoid bubbles/silver streaks; drying optional for well‑stored material
  Drying time 2‑4 h  
Injection Rear zone 160‑180 Narrow processing window; strictly avoid>210‑230℃, formaldehyde gas will be generated by decomposition
  Middle zone 170‑200  
  Front zone 190‑210  
  Nozzle temperature 180‑210 Slightly lower or close to front zone to prevent drooling
  Melt temperature (POM‑C) 190‑210 Do not exceed 210℃ for copolymer POM
  Mold temperature 80‑105 Higher mold temp improves crystallization, dimensional stability, gloss & reduces sink marks; up to 120℃ for thin‑wall / long‑flow complex parts
  Injection pressure 70‑120 MPa 120‑140 MPa for small‑gate, thin‑wall long‑flow parts
  Hold‑up pressure 50‑100 MPa Longer hold‑time for thicker wall to reduce shrinkage
  Back pressure 0.5‑2.0 MPa Keep low; excessive back‑pressure causes shear‑heating degradation
  Injection speed Medium‑high Fast for thin‑wall; slow for thick‑wall to avoid jetting
  Screw speed 60‑90 rpm Avoid excessive shear heat
  Barrel residence time <20‑30 min Short residence required; max 1 h at 190℃
  Short‑term shutdown Drop barrel temp to 150 Clean barrel for long‑term shutdown
  Barrel purging material PE / PP Do NOT use PVC or halogen‑containing polymers
Post‑treatment Annealing (optional) 120‑130, 2‑4 ℃‑h For high‑precision / non‑ambient‑use parts; add ~10 min per 1 mm wall thickness

Note: All information above is for reference only!