TPU Covestro 487
TPU Covestro 487
TPU Covestro 487 is thermoplastic polyurethane elastomer with outstanding mechanical properties, good heat resistance, excellent oil‑resistance and hydrolysis‑resistance.
Main Applications
Automotive engineering components: seals, damping elements. Industrial applications: roller coating parts, seals, films. Machine parts: functional components for mechanical engineering & plant equipment.
Physical Properties
| Property Category | Item | Test Condition | Test Standard | Typical Reference Data | Unit |
|---|---|---|---|---|---|
| Physical Properties | Density | — | ISO 1183 | 1.21 | g/cm³ |
| Mechanical Properties | Shore Hardness | — | ISO 868 | 86 | Shore A |
| Tensile strength at break | — | ISO 37 | 35 | MPa | |
| Elongation at break | — | ISO 37 | 500 | % | |
| 100% Modulus | — | ISO 37 | 6 | MPa | |
| 300% Modulus | — | ISO 37 | 14 | MPa | |
| Flexural Modulus | — | ISO 178 | 30 | MPa | |
| Tear propagation strength | — | DIN 53515 | 70 | kN/m | |
| Abrasion loss | — | ISO 4649 | 20 | mm³ | |
| Rebound resilience | — | ISO 4662 | 45 | % | |
| Compression Performance | Compression set | 70h / 22℃ | ISO 815 | 40 | % |
| Compression set | 70h / 70℃ | ISO 815 | 25 | % |
Processing Parameters
| Process | Parameter | Unit | Reference Range | Remarks |
|---|---|---|---|---|
| Pre‑drying | Drying temperature | ℃ | 80‑110 | Circulating hot‑air drying recommended; TPU is moisture‑sensitive, drying is mandatory |
| Drying time | h | ≥3 | Until moisture<0.05% | |
| Material bed thickness | mm | ≤30 | Guarantee drying efficiency | |
| Injection molding | Rear feed zone temp | ℃ | 175‑195 | Avoid long‑term melt residence under high temperature |
| Middle compression zone temp | ℃ | 180‑200 | ||
| Front metering zone temp | ℃ | 185‑205 | ||
| Nozzle temperature | ℃ | Equal‑to‑slightly lower than front zone | Prevent drooling or cold‑plug blockage | |
| Melt temperature | ℃ | 190‑210 | Strictly prohibit>240℃ to avoid degradation | |
| Mold temperature | ℃ | 20‑40 | Lower mold temp shortens cycle time & reduces sticking | |
| Injection pressure | bar | 50‑100 | Keep as low as possible while full filling | |
| Hold‑pressure | bar | 30%‑60% of injection pressure | Excessive hold‑pressure & long hold‑time shall be avoided to reduce internal stress | |
| Screw speed | rpm | 50‑100 | High speed causes shear overheating | |
| Back pressure | bar | 5‑15 | Improve melt homogeneity; excessive back‑pressure generates extra heat |
Note: All information above is for reference only!